Boeing Test Results

SPC-901 NEUTRAL BOEING D6-17487 REV.N TEST RESULTS

  • SAFE to use on Magnesium substrate
  • SMI tested Sandwich Corrosion Test – Conforms
  • Hydrogen Corrosion Test – Conforms
  • Immersion Corrosion Test – Results Table Below

Weight Change (per 1″ x 2″ panel)
Specimen Max. Allowed FOUND
Clad 2024-T3 Aluminum (AMS 4041) +/-10 mg 0.1 mg
Bare 2024-T3 Aluminum (AMS 4037) Alodined per MIL-C-5541 +/-10 mg0.6 mg
Bare 2024-T3 Aluminum (AMS 4037) Anodized per MIL-A-8625 Type I sealed per BAC 5019 class 3 +/-10 mg+ 0.1 mg
Bare 7075-T6 Aluminum (AMS 4045) Anodized per MIL-A-8625 Type I sealed per BAC 5019 class 3 +/-10 mg+ 0.5 mg
130 Steel, cad plated, baked, and postplate treated per BAC 5804 +/-10 mg3.7 mg
4130 Steel, cadmium plated, per BAC 5701 (QQ-P-416, Ty1 CI1) +/-10 mg+ 0.8 mg
6AI-4V Titanium per MIL-T-9046 (AMS 4911) +/-10 mg0.5 mg
QQ-M-44 Magnesium (AMS 4376) dichromate treated per MIL-M-3171 Ty III (scribed panel) +/-20 mg12.2 mg
4130 Steel (AMS 6350) MIL-S-18729 +/-30 mg+ 0.1 mg

SPC-909 NEUTRAL BOEING D6-17487 REV.N TEST RESULTS

  • NOT for use on Magnesium substrate
  • SMI tested
  • Sandwich Corrosion Test – Conforms
  • Hydrogen Corrosion Test – Conforms
  • Immersion Corrosion Test – Results Table Below

Weight Change (per 1″ x 2″ panel)
Specimen Max. Allowed FOUND
Clad 2024-T3 Aluminum (AMS 4041) +/-10 mg0.1 mg
Bare 2024-T3 Aluminum (AMS 4037) Alodined per MIL-C-5541 +/-10 mg0.9 mg
Bare 2024-T3 Aluminum (AMS 4037) Anodized per MIL-A-8625 Type I sealed per BAC 5019 class 3 +/-10 mg+ 0.1 mg
Bare 7075-T6 Aluminum (AMS 4045) Anodized per MIL-A-8625 Type I sealed per BAC 5019 class 3 +/-10 mg+ 0.2 mg
130 Steel, cad plated, baked, and postplate treated per BAC 5804 +/-10 mg6.0 mg
4130 Steel, cadmium plated, per BAC 5701 (QQ-P-416, Ty1 CI1) +/-10 mg< 0.1 mg
6AI-4V Titanium per MIL-T-9046 (AMS 4911) +/-10 mg+ 0.3 mg
QQ-M-44 Magnesium (AMS 4376) dichromate treated per MIL-M-3171 Ty III (scribed panel) +/-20 mgNOT TESTED
4130 Steel (AMS 6350) MIL-S-18729 +/-30 mg1.1 mg